    I had a rather exciting incident trying to pour aluminum into paper towel tubes to make round bar for the lathe. It was just plain sand that got a bit of
    Message 1 of 27 , Mar 13, 2013
      I had a rather exciting incident trying to pour aluminum into paper towel
      tubes to make round bar for the lathe. It was just plain sand that got a
      bit of moisture in it sitting out over night. I stuffed the tube in and
      poured sand around it. When I poured the aluminum in it made a nice poof
      and blew sand and molten aluminum out of the hole. It burned holes in my
      leathers and made me do a dance, but I wouldn't exactly call it an
      explosion. No bang, no shock wave felt. Pyroclastic even for sure but not
      an explosion.
      Did I say it scared the shit out of me?? ;)

      Glenn
      ----- Original Message -----
      From: "David Patterson" <odd_kins@...>
      To: <hobbicast@yahoogroups.com>
      Sent: Tuesday, March 12, 2013 10:18 PM
      Subject: Re: [hobbicast] Damp molds ( observation and question)


      Nelson that's not even close to what we're talking about. Pouring metal into
      water has been done since before you were born.
      We're talking about a closed mold that has excess water in the sand. In the
      case I was refering to was an over wet drag, in just one area. the mold is
      pour fast and the moist sand covered quickly enough to not allow the steam
      to escape the mold fast enough to prevent the mold from exploding.
      With that in mind, is why I make only the molds I'm going to pour that day.

      Dave Patterson
      odd_kins@...
      http://home.comcast.net/~oddkins/foundry_home.html

      --- On Tue, 3/12/13, Nelson Collar <nel2lar@...> wrote:


      From: Nelson Collar <nel2lar@...>
      Subject: Re: [hobbicast] Damp molds ( observation and question)
      To: "hobbicast@yahoogroups.com" <hobbicast@yahoogroups.com>
      Date: Tuesday, March 12, 2013, 9:55 PM







      I went to UTube for some of the stupid guys doing what you say is so
      dangerous:

      http://www.youtube.com/watch?v=Pkfyj42f6EU
      http://www.youtube.com/watch?v=x4sTS5uvWOM
      http://www.youtube.com/watch?v=HWUF6wuYDt0

      ________________________________
      From: David Patterson <odd_kins@...>
      To: hobbicast@yahoogroups.com
      Sent: Tuesday, March 12, 2013 11:51 PM
      Subject: Re: [hobbicast] Damp molds ( observation and question)



      Jeshua, I have to agree with you. I have only seen one steam explosion
      during the time I worked for at a local foundry. luckly no one was hurt, as
      all were wearing safety equipment.
      Water enter the mold from a leak in the roof, dropped into a riser so no one
      knew it soaked the sand. The mold did blow sand and aluminum out of the mold
      far enough to destroy other molds and could have hurt those nearby, not by
      the explosion but by liquid metal falling all around.

      Dave Patterson
      odd_kins@...
      http://home.comcast.net/~oddkins/foundry_home.html

      --- On Tue, 3/12/13, Jeshua Lacock <jeshua@...> wrote:

      From: Jeshua Lacock <jeshua@...>
      Subject: Re: [hobbicast] Damp molds ( observation and question)
      To: hobbicast@yahoogroups.com
      Date: Tuesday, March 12, 2013, 8:35 PM



      On Mar 12, 2013, at 9:30 PM, Nelson Collar wrote:

      > Well I can say I am no newbie. I've cast more years than you wiped your
      > own nose. I have had too wet sand and the danger is the metal spilling out
      > of the mold and blow holes where the gas from the excessive water could
      > not fill because of steam. NO it is not a dangerous. Some of you all get a
      > little bit of knowledge and think you know it all. This group is not what
      > it was years ago. Wonk what keep you around?

      How do you know you have cast more years than I have wiped my nose? I am no
      newbie either. I too have poured on wet sand.

      But yeah water and molten metal are totally safe. No possibility of
      explosions. No one has ever been maimed or killed or anything. No need to be
      cautious.

      Get real.

      The reason why you have been able to pour on wet sand is because the a. sand
      helps, and b. there must have not been enough pressure built up. Confine
      some steam and you have serious danger.

      Sincerely,

      Jeshua Lacock
      Founder/Engineer
      3DTOPO Incorporated
      <http://3DTOPO.com>
      Phone: 208.462.4171

      [Non-text portions of this message have been removed]

      [Non-text portions of this message have been removed]








      [Non-text portions of this message have been removed]



      ------------------------------------

      For discussion of Metal Casting and related issues
      this list does not accept attachments.

      Files area and list services are at:
      http://groups.yahoo.com/group/hobbicast

      For additional files and photos and off topic discussions
      check out these two affiliated sites:
      http://groups.yahoo.com/group/sandcrabs
      http://groups.yahoo.com/group/Hobbicast1

      Please visit our sponsor: Budget Casting Supply
      http://budgetcastingsupply.com/

      List Owner:
      owly@...

      Yahoo! Groups Links
    Your message has been successfully submitted and would be delivered to recipients shortly.