  • Ray Brandes
    All my early work was done using cans. I found that hammering them into a tight chunk allowed me to put 4 or 5 in my 3 pipe cap crucible. These were melted in
    Message 1 of 46 , Jan 24, 2002
      All my early work was done using cans. I found that hammering them into
      a tight chunk allowed me to put 4 or 5 in my 3" pipe cap crucible. These
      were melted in an electric kiln. Smoke is right about the smoke (thus
      his nick name) and the dross. However, the castings came out great and
      took a very nice polish.
      These days I use 6061 chips from the shop. I put a #30 crucible in my
      furnace and just keep dumping in the chips until the level gets high
      then I do a dip-out into ingot molds. Last session yielded 75 lbs of
      ingots.
      The job I am doing now removes 70% of the metal so I decided early to
      reclaim the scrap. Before I started I cleaned the machine compleatly and
      the floor all around got swept and vacuumed. Now everything I picked up
      would be aluminum chips. I have 3 pails of the stuff so far to add to my
      stockpile. I may never have to buy scrap again!
      Ray in FLA

      Smoke wrote:
      >
      > DO NOT toss in soft drink cans!!!!!
      >
      > I melted a whole !#$%^%^pot full of them last summer. They put off a lot of
      > smoke from the burning paint, and you'll get way to much dross and garbage
    • Steven DePhillips
      About 3-4 months ago in Georgia they passed a law that the scrap yards can only pay in check after making a copy of your drivers licence and licence plate
      Message 46 of 46 , Dec 7, 2012
        About 3-4 months ago in Georgia they passed a law that the scrap yards can only pay in check after making a copy of your drivers licence and licence plate numbers. But the big thing is you cant scrap any AC units without an HVAC licence, large quantity's of copper pipes without a Plumbing licence and large quantity's of copper wire without an being an Electrician. They say it is to stop copper theft.   


        ________________________________
        From: Nelson Collar <nel2lar@...>
        To: "hobbicast@yahoogroups.com" <hobbicast@yahoogroups.com>
        Sent: Tuesday, December 4, 2012 8:34 PM
        Subject: Re: [hobbicast] Al cans


         
        Some of the time and if they do not see them. My are even a spike they reject.

        ________________________________
        From: Nick Andrews <nickjandrews@...>
        To: hobbicast@yahoogroups.com
        Sent: Tuesday, December 4, 2012 8:12 PM
        Subject: Re: [hobbicast] Al cans

        None of that yet where I go here, but they do have a new poster up
        regarding stolen railroad scrap and reporting it.  I have a small piece of
        rail and maybe a spike plate laying around, but I doubt they would raise an
        eyebrow if I took them in, with all the various building salvage and such I
        take them.

        On Tue, Dec 4, 2012 at 6:46 PM, StoneTool <owly@...> wrote:

        > **
        >
        >
        > It's already reached that point here........most scrap yards while they
        > may pay in cash, demand identification and a signature. They have to
        > cover themselves in case someone is selling stolen property. For
        > example, someone stole over a hundred radiators out of a friend's
        > salvage yard, and we were able to catch the guy because he sold them and
        > the salvage yard had a record of the sale.
        >
        > Howard
        >
        > On 12/04/2012 04:00 PM, geoffrey_roberts@... wrote:
        > > i am trying to make some money; things are very tight here. i know
        > there's a recession but in this part of Florida things are very, very
        > tough. By law, copper wire is not sold in scrap yards because is it "hot."
        > >
        > > i am sorry to learn about the British. It probaby will be it the US
        > soon. Thank you all (my southern accent is showing) justgeoff
        > >
        > >
        > >
        > > ------------------------------------
        > >
        > > For discussion of Metal Casting and related issues
        > > this list does not accept attachments.
        > >
        > > Files area and list services are at:
        > > http://groups.yahoo.com/group/hobbicast
        > >
        > > For additional files and photos and off topic discussions
        > > check out these two affiliated sites:
        > > http://groups.yahoo.com/group/sandcrabs
        > > http://groups.yahoo.com/group/Hobbicast1
        > >
        > > Please visit our sponsor: Budget Casting Supply
        > > http://budgetcastingsupply.com/
        > >
        > > List Owner:
        > > owly@...
        > >
        > > Yahoo! Groups Links
        > >
        > >
        > >
        > >
        >

        >

        --
        Nick A

        "You know what I wish?  I wish that all the scum of the world had but a
        single throat, and I had my hands about it..."  Rorschach, 1975

        "They that can give up essential liberty to obtain a little temporary
        safety deserve neither liberty nor safety."- Benjamin Franklin, Historical
        Review of Pennsylvania, 1759

        "Suburbia is where the developer bulldozes out the trees, then names the
        streets after them." Bill Vaughan

        "The price of apathy towards public affairs is to be ruled by evil men."
        Plato

        [Non-text portions of this message have been removed]

        ------------------------------------

        For discussion of Metal Casting and related issues
        this list does not accept attachments. 

        Files area and list services are at:
            http://groups.yahoo.com/group/hobbicast

        For additional files and photos and off topic discussions
        check out these two affiliated sites:
            http://groups.yahoo.com/group/sandcrabs
            http://groups.yahoo.com/group/Hobbicast1

        Please visit our sponsor: Budget Casting Supply
        http://budgetcastingsupply.com/

        List Owner:
        owly@...

        Yahoo! Groups Links

        [Non-text portions of this message have been removed]




        [Non-text portions of this message have been removed]
      Your message has been successfully submitted and would be delivered to recipients shortly.