4625Re: Toyoba Printight 152 / Rigilon MX II 145 / BASF WS 152

Expand Messages
  • elumdesigns
    Sep 1, 2005
      I am using the Orbital X as well:
      Rigilon MX II 145
      Exposure 1 min 20 sec
      4.5 to 5 minute washout @ 90 degrees
      10 minutes drying time @ 165 degrees (need to check temp to be exact.)
      10 minute postexposure

      Rigilon HX 145
      Exposure 2 - 3 minutes depending on application and how much shoulder
      we need
      4 minute washout @ 90 degrees
      10 minutes drying time @ 165 degrees (need to check temp to be exact.)
      15 minute postexposure

      Miraclon MS 145
      Exposure 1 min 45 sec
      5 minute washout @ 90 degrees
      10 minutes drying time @ 165 degrees (need to check temp to be exact.)
      10 minute postexposure

      BASF WS152
      Exposure 2 min 30 sec
      10 minute washout @ 90 degrees
      10 minutes drying time @ 165 degrees (need to check temp to be exact.)
      15 minute postexposure




      --- In PPLetterpress@yahoogroups.com, "Gerald Lange" <bieler@w...> wrote:
      > Brad
      >
      > What is the sequence you use for the Rigilon? I think it would be
      > useful for folks to provide their "successful" sequences here. Of
      > course they would need to be very specific to be of any use to others:
      > Machine. Manufacturer/Brand/Formulation Code. Exposure time, washout
      > time, drying time, post-exposure time. Purpose. Even sources would be
      > good.
      >
      > For instance (with my A&V Orbital machine) running Toyobo Printight
      > 152 GRs (steel-backed), which I buy from A&V, I have a generic
      > sequence for deep impression as 6 minutes exposure, 5 minutes washout
      > (90 degrees F), 15 minutes drying time (150 degrees F) and 12 minutes
      > post-exposure. I modify this a bit per client dependent upon their
      > intended use and practices.
      >
      > Gerald
    • Show all 19 messages in this topic